| 规格级别 | 其它 其它 其它 | 外观颜色 | |
| 该料用途 | 面包袋,高密度聚乙烯瓶套,特种混合 | ||
| 备注说明 | 涂膜性能。特点:低凝胶,清晰度好,易加工性。 | ||
| 性能项目 | 试验条件[状态] | 测试方法 | 测试数据 | 数据单位 | |
| 基本性能 | 密度 | ASTM D-792 | 0.923 | g/cm3 | |
| 熔体流动速率 | 190℃/2.16 kg | ASTM D-1238 | 1.4 | g/10min | |
| 透湿 | ASTM D-1434 | 0.35 | |||
| 透氧 | 120 | ||||
| 机械性能 | 拉伸屈服强度 | MD | ASTM D-882 | 16 | MPa | 
| 拉伸屈服强度 | TD | ASTM D-882 | 12 | MPa | |
| 埃尔曼多夫撕裂强度 | MD | ASTM D-1922 | 4 | g | |
| 埃尔曼多夫撕裂强度 | TD | ASTM D-1922 | 18 | g | |
| 断裂伸长率 | MD | ASTM D-882 | 600 | % | |
| 断裂伸长率 | TD | ASTM D-882 | 900 | % | |
| 落锤冲击 | ASTM D-1709 | 2 | g/micron | ||
| 割线模量 | MD | ASTM D-882 | 0.2 | GPa | |
| 割线模量 | TD | ASTM D-882 | 0.26 | GPa | |
| 摩擦系数 | ASTM D-882 | 0.2 | |||
| 拉伸断裂强度 | MD | ASTM D-882 | 42 | MPa | |
| 拉伸断裂强度 | TD | ASTM D-882 | 32 | MPa | |
| 热性能 | 维卡软化点 | ASTM D-1525 | 96 | ℃ | |
| 脆化温度 | ASTM D-696 | -68 | ℃ | ||
| 光学性能 | 雾度 | ASTM D-1003 | 8 | % | |
| 光泽度 | ASTM D-1894 | 57 | % | ||